Polyaspartic DTM

Formula date: Nov 20, 2025

Component

F520/F420/GB930-100/GB902-100.

Curing method

Air drying.

Application

DTM.

Characters

High solid content, fast drying.

A component

Material Content
F520(Desmophen NH 1520 Equivalent) 20
F420(Desmophen NH 1420 Equivalent) 20
BYK163 Dispersant1
4200 Wax paste2
Rutile titanium dioxide35
Zinc phosphate10
R972 fumed silica0.4
3A Molecular sieve3
BYK1790 defoaming agent0.2
BYK-410 Rheology agent0.1
EFKA3600 Leveling agent0.1
F421-FW200 Black paste0.3
1130 UV absorber0.9
292 UV absorber0.6
A-187 silane coupling agent1
n-Butyl acetate2.9
PMA2.5

B component

Material Content
HT60068
Dehydrating agent0.5
N-Butyl acetate16
PMA15.5

Ratio

A:B=2.5:1 by weight

Specifications

Pot life>40min
Solid content≥85%
Touch dry time 25℃≤1h
Hard dry time 25℃≤3h
Thickness100-150µm or according to actual needs
HardnessH
Glossness≥85°
Elongation<20%
Aging resistanceUVA≥2000h
Salt spray resistance>500h

Construction description

High-pressure airless spraying or manual spraying is recommended. Roller coating or brush coating can also be used.

Feiyang Protech has been specializing in the production of raw materials for polyaspartic coatings for 30 years and can provide polyaspartic resins, hardeners and coating formulations. Feel free to contact us: [email protected]

Our products list:

Consult our engineers to customize a coating formulation for your project. Contact our Tech Team

Similar Posts